ASTM D3410 - Measuring the Compressive Strength of Polymer Matrix Composites

ASTM D3410 compression testing of composite polymers

ASTM D3410 is a testing standard that determines the in-plane compressive properties of polymer matrix composite materials reinforced by high-modulus fibers. This test method is designed to produce compressive property data on CFRP’s (Carbon Fiber Reinforced Polymers) mainly used by the Aerospace industry for material specifications, research and development, quality assurance, and structural design and analysis. Carbon fiber reinforced polymers are a preferred material whenever high strength-to-weight ratio and stiffness (rigidity) is required, such as when building aircraft, ships, and automotives, as well as in civil engineering. CFRPs are also being used in an increasing number of consumer and technical applications, such as in sporting equipment.

The compressive force is being introduced by shear loading with wedge grip faces inside a loading fixture. Important results obtained during this test are the ultimate compressive strength, compressive and ultimate compressive strain, the compressive Chord modulus of elasticity, compressive Poisson’s ratio by chord modulus and the transition strain.

Test Fixture

ASTM D3410 testing requires an S4690A IITRI Compression Fixture, which is placed between two platens - a spherical platen on top, and a rigid one on the bottom. Through the wedge action of the test fixture, the compressive force is initiated through shear onto the specimen, (different than the end loading in ASTM D695, for example).

ASTM D3410 test fixture

Materials Testing System

This test is best performed on a high force universal testing system such as Instron's 6800 Series along with an AlignPRO fixture. Though a 250 kN capacity system is usually sufficient for composites, a higher capacity system may be preferred for labs who perform a wide variety of high force testing.



ASTM D3410 Test Setup
6800 Series
Bluehill Universal Software
AlignPro
2580 Series Load Cell
S4690A IITRI Compression Fixture

 

ASTM D3410 test setup
Testing Tips and Tricks
  • Compression modulus, and especially ultimate compressive stress, are sensitive to poor material fabrication practices, damage induced by improper specimen machining, and lack of control of fiber alignment.
  • The data resulting from ASTM D3410 has been shown to be sensitive to the flatness and parallelism of the specimen tabs, so care should be taken to ensure that the specimen tolerance requirements are met. This usually requires precision grinding of the tab surfaces after bonding them to the specimen.
  • The surface finish of the mating surface of the wedge grip assembly can have a significant effect on test results. Since these surfaces undergo sliding contact, they must be polished, lubricated, and nick-free.
Related Content

Série 6800 Systèmes d'essai universels

Les systèmes d'essais universels Instron série 6800 offrent une précision et une fiabilité inégalées. Construit sur une architecture système Operator Protect en instance de brevet avec un tout nouveau kit de régulation d’air Smart-Close et des fonctions d’atténuation des collisions, la série 6800 rend les essais de matériaux plus simples, plus intelligents et plus sûrs que jamais.

Brochure sur les essais de composites

Les machines de test universelles d’Instron sont conçues pour effectuer les types de essais les plus couramment utilisés dans l’industrie des composites, y compris, mais sans s’y limiter, la traction dans le plan, la traction dans l’épaisseur, le cisaillement interlaminaire, la compression en fin, le cisaillement ou la charge combinée, et la compression après impact.

Brochure Bluehill Universal

Le logiciel Bluehill Universal est intégralement conçu pour une interaction tactile et une expérience utilisateur intuitive. Vous découvrirez que les essais deviennent plus simples et plus intelligents grâce à des fonctionnalités, telles que les méthodes d’essais préconfigurées, le QuickTest fait en quelques secondes, l’exportation de données optimisée et Instron Connect - une nouvelle fonctionnalité qui fournit un lien de communication direct avec le service technique. Les utilisateurs des versions précédentes du logiciel, telles que Bluehill 2 et Bluehill 3, peuvent facilement faire la mise à jour à la toute dernière version de Bluehill.

Dispositifs d’essai des composites - compression

Instron propose plusieurs dispositifs pour les essais de compression des composites sans plaques de guidage anti-flambage. C’est souvent le moyen privilégié pour les essais sur composites, car la longueur libre non supportée est plus représentative du véritable comportement en compression.