EN 1465 Adhesives Lap Shear Bond Strength of Rigid-to-Rigid Assemblies

Written by Meredith Bernstein

EN 1465 test setup

EN 1465 is a tensile test used to measure the adhesive lap-shear bond strength of rigid-to-rigid assemblies. This standard is used by many industries to test adhesives applied to materials such as metals, plastics, wood, and composites. Lap-shear strength is a critical characteristic of any adhesive, as they can exhibit unique shear properties.

How Does it Differ from ISO 4587?

EN 1465 is extremely similar to ISO 4587 with the exception of test rate. Both standards use identical test setups, specimen geometries, and results reporting, with the exception that ISO 4587 calls out a specific test rate of 8.3MPa to 9.8MPa while EN 1465 only specifies a constant rate of load application. Both standards state that the average specimen should break in a period of 65+/-20 sec.

Materials Testing System

EN1465 is performed on a universal testing machine with a system capacity dependent on the strength of the adhesive. Most tests to this standard will fall into the capacity range between 1 kN and 5 kN, making this application perfect for a single column test frame such as Instron's 34SC or 68SC. If the adhesive requires a higher capacity system, Instron’s dual column table model frames are available up to 50 kN.

En 1465 test setup

EN 1465 Test Setup

1. Instron 34SC-05

2. Bluehill Universal Dashboard (2490-696)

3. 2530 Series Load Cell (2530-100N)

4. 500 N Screw Side-Action Grips (2710-112)

 

 

Grips

Both pneumatic side-action grips and advanced screw side-action grips are excellent gripping choices for this standard. Both types of grips are adjustable in order to offset the jaw faces and ensure that the lap joint remains centered, and both feature quick-change jaw faces that can be easily changed to accommodate different materials.

5 kN Model | 2712-045
1 kN Model | 2710-113

Helpful Tips and Tricks

  • When testing lap shear specimens, the lap joint causes the two ends of the specimen to be offset from the vertical load line of the test. In order to ensure that the specimen remains centered in the load string and yields a true shear force calculation, the grips must have offset jaw faces to ensure they are directly aligned with the plane of the adhesive bond.
  • EN 1465 requires reporting the breaking force or strength, however, it is important to remember that shear strength is calculated by dividing the breaking force by the adhesive bond area.
  • Users who purchase Instron's Bluehill Universal software are provided with one free application module upon purchase. Each module contains pre-configured test methods and supporting documentation to assist with testing to various standards, including EN 1465 which is part of the Adhesives module.

Related Content

6800 Series Premier Testing Systems Brochure

Instron 6800 Series Universal Testing Systems provide unparalleled accuracy and reliability. Built on a patent-pending Operator Protect system architecture with an all-new Smart-Close Air Kit and Collision Mitigation features, the 6800 Series makes materials testing simpler, smarter, and safer than ever before.

3400 Series - Affordable Testing Solutions

Instron 3400 Series Universal Testing Systems for Tensile, Compression, Bend, and other material property tests.

Bluehill Universal Brochure

Bluehill Universal Software is built from the ground-up for touch interaction and an intuitive user experience. Discover simpler and smarter testing with features such as pre-loaded test methods, QuickTest in seconds, enhanced data exporting: and Instron Connect – a new feature that provides a direct communication link to Service. Users of previous versions of software such as Bluehill 2 and Bluehill 3 can easily upgrade to the newest version of Bluehill.

2712-04X Series Pneumatic Side-Action Grips

Pneumatic side-action grips offer a versatile gripping solution for a wide range of materials. Rated capacities between 1 and 10 kN.

2710 Series Screw Side Action Grips

Screw side action grips provide a simple and effective method for holding test specimens and can be used in a wide range of applications.